Battery Cell Benchmarking Teardown: Complete Guide
A battery cell benchmarking teardown takes a commercial or competitor cell apart in a controlled way and measures every component, so you know how it is built and how it performs. A full teardown covers baseline tests, safe opening, component measurements, materials and electrolyte analysis, and often rebuilding small cells from the harvested electrodes.
This guide is for cell design, product strategy and competitive intelligence teams who want to commission or run a teardown. It walks through each stage, lists the metrics that matter and the deliverables to expect, and explains what a teardown cannot tell you.
Benchmarking teardown vs failure analysis
Both open cells, but for different reasons. A benchmarking teardown studies healthy cells to learn design choices: materials, loadings, thicknesses and construction. Failure analysis studies cells that failed or aged badly to find a root cause.
If you are dealing with failed cells, see our post-mortem lab workflow instead. This guide covers benchmarking only.
Stage 1: Plan the scope
Start with the questions, not the techniques. Typical questions are: what energy density does the cell reach and how? What materials are used? How thick are the electrodes and how heavily loaded? How is the cell constructed and sealed?
- Decide which questions matter and which are out of scope.
- Agree how many cells to buy, and buy them through normal channels with records.
- Decide whether to benchmark against your own cell side by side.
- Agree confidentiality and data ownership with the lab (see protecting IP when outsourcing tests).
Stage 2: Non-destructive baseline
Measure everything you can before opening the cell, because opening destroys it.
- Dimensions and mass: the basis for energy density by weight and volume.
- Capacity and voltage curves: at set rates and temperatures.
- Resistance and impedance: DC internal resistance and EIS for power capability.
- X-ray CT: internal layout, electrode alignment, overhang and tab design, without opening.
Stage 3: Safe discharge and opening
The cell is fully discharged, then opened in an inert atmosphere such as an argon glovebox, because lithiated electrodes and electrolyte react with air and moisture. Every layer is photographed and documented as it comes out. Opening cells is hazardous and must only be done by trained staff with proper equipment.
Stage 4: Component measurements
This is the core of a battery cell benchmarking teardown. Each component is separated, cleaned where needed and measured:
- Electrodes: total and coating thickness, coated area, coating mass per area (areal loading), single- or double-sided.
- Density and porosity: calculated from loading, thickness and material densities.
- Current collectors: foil material and thickness.
- Separator: thickness, type and any coating.
- Construction: number of layers or jelly-roll length, tab design and welding, casing or pouch material.
Stage 5: Materials and chemistry
Samples of each electrode are analysed to identify materials:
- SEM: particle size, shape and coating structure.
- EDS: elements present at the surface.
- XRD: crystal structure of the active materials.
- ICP: bulk elemental composition, for example the nickel, manganese and cobalt ratio in a cathode.
Canrud runs SEM and GC-MS root cause investigations, and the same tools apply to benchmarking.
Stage 6: Electrolyte analysis
Electrolyte evaporates and degrades once the cell is open, so it should be recovered early, often from a dedicated cell. Gas chromatography with mass spectrometry (GC-MS) identifies the solvents and many additives. The salt is usually identified separately. Electrolyte composition often explains differences in life and low-temperature performance between cells that look similar.
Stage 7: Rebuild and benchmark components
Harvested electrodes can be rebuilt into coin or small pouch cells and tested against your own materials under the same conditions. This separates the effect of each component from the effect of the whole cell design. Benchmarking specialists such as FEV describe this rebuild step as part of their own process.
The benchmark metrics table
|
Metric |
How it is measured |
Why it matters |
|---|---|---|
|
Energy density (Wh/kg, Wh/L) |
Capacity, voltage, mass and volume |
Headline comparison between cells |
|
Areal loading |
Coating mass per area |
Sets capacity per layer and power trade-off |
|
Electrode thickness and density |
Micrometer, cross-section, calculation |
Shows how hard the electrodes were calendered |
|
Porosity |
From density, or by measurement |
Affects rate capability and electrolyte access |
|
Cathode composition |
ICP, XRD |
Shows chemistry and supplier choices |
|
Particle morphology |
SEM |
Indicates material grade and processing |
|
Electrolyte composition |
GC-MS |
Explains life and temperature behaviour |
|
Inactive mass share |
Weighing each component |
Shows how efficiently the cell is packaged |
|
Internal layout |
X-ray CT |
Reveals overhang, alignment and tab design |
What should the teardown report include?
- Scope, number of cells and how they were sourced.
- Baseline electrical results and CT images.
- Photographs of every layer during opening.
- A bill of materials with mass and volume share for each component.
- Electrode, separator and foil measurements.
- Materials and electrolyte analysis results.
- Rebuilt-cell results, if in scope.
- Raw data files, not only summary charts.
What a teardown cannot tell you
A teardown shows what is in a cell, not exactly how it was made. Process settings such as drying, formation and ageing can only be inferred. A few cells may not represent a whole production run. Results also reflect the cells you bought, which may differ from the supplier's latest version. Treat conclusions about manufacturing as estimates, and take legal advice on how you obtain cells and use the results.
For an example of how an established benchmarking provider describes its process, see FEV's battery cell benchmarking overview.
Cylindrical, prismatic or pouch: what changes in a teardown?
|
Format |
How it is opened |
What to watch |
|---|---|---|
|
Cylindrical |
Cut the can at the ends or along its length, then unwind the jelly roll |
Tension in the roll, central pin or hollow core, tab positions along the electrode |
|
Prismatic |
Open the aluminium or steel case, then remove the stacked or wound core |
Vent design, insulation sheets, tab and busbar welds |
|
Pouch |
Cut the pouch film around the edge and lift out the stack |
Sealing width, tab sealant, layer count and alignment |
Each format needs its own tools and safety steps. Cylindrical cells hold the electrodes under tension, and opening the can can release electrolyte and debris quickly, so labs work slowly and in an inert atmosphere.
How do you turn measurements into a design comparison?
The numbers become useful when you compare them side by side with your own cell or a second competitor. Three views are especially helpful:
- Mass breakdown: the share of total cell mass in cathode, anode, foils, separator, electrolyte and casing. A low inactive-mass share usually means good packaging efficiency.
- Electrode design: loading, thickness and porosity of each electrode, which show where the designer traded energy for power.
- Materials: composition and particle features, which hint at material grade and supplier.
Present the comparison in one table per view, with the measurement method and number of samples next to each value, so readers know how much to trust it.
Should you run a teardown in-house or use a lab?
Running teardowns in-house makes sense if you do them often and already have a glovebox, imaging and chemistry instruments, and trained staff. Using an outside lab makes sense if teardowns are occasional, if you need instruments you do not own, or if you want an independent report to share with partners. Many teams do the non-destructive baseline themselves and send cells out for opening and analysis.
How do you keep a teardown safe?
Opening lithium-ion cells carries real risks: short circuits during opening, reactive lithiated anode material, flammable electrolyte and, for some salts, toxic decomposition products such as hydrogen fluoride. A safe teardown follows a written procedure:
- Discharge fully and confirm the voltage before cutting.
- Use insulated, non-sparking tools and cut away from the electrode stack.
- Work in an inert-atmosphere glovebox or a controlled dry room with extraction.
- Keep fire suppression suited to lithium batteries close by.
- Dispose of electrodes, electrolyte and casings as hazardous waste.
What drives the time and effort of a teardown?
Scope drives effort more than anything else. A teardown limited to dimensions, mass and electrode measurements is far smaller than one that adds full materials analysis, electrolyte work and rebuilt cells. Cell format matters too: large prismatic cells take longer to open and sample than small cylindrical ones. The number of cells and repeats, and how detailed the report must be, complete the picture. Defining the questions in stage 1 is the best way to keep effort focused.
Common mistakes when commissioning a teardown
- No baseline before opening: electrical data and CT images cannot be collected once the cell is open.
- Too few cells: one cell cannot show variation, and there is none left for electrolyte recovery.
- Vague questions: a report that measures everything but answers nothing specific.
- Summary charts only: without raw data you cannot compare future teardowns.
- Ignoring cell history: storage time and conditions affect what you find, so record them.
|
Want to see inside a competitor cell? Tell us which cell, how many samples and what you need to learn, and request a teardown quote from Canrud. Scope is agreed on a short call, all costs listed upfront. |
Frequently asked questions
How many cells do I need for a benchmarking teardown?
More than one. You need cells for non-destructive tests, at least one for a full teardown, and ideally one opened only to recover electrolyte. Extra cells let you check whether what you found is typical or a one-off. Agree the number with the lab based on the questions you want answered.
Is it legal to tear down a competitor's cell?
Taking apart a product you bought legally is common practice for benchmarking, but how you obtained the cells and how you use the results can raise legal questions, for example around contracts or patents. Take legal advice before you start, especially if results will guide your own product design.
Can a teardown reveal how a cell was manufactured?
Only partly. A teardown shows the result of manufacturing: materials, loadings, thicknesses and construction. It cannot show process settings such as mixing time, drying conditions or the formation protocol. Some can be inferred from the evidence, but treat those conclusions as informed estimates, not facts.
What is the difference between a teardown and a post-mortem?
A benchmarking teardown studies healthy cells to learn how they are designed and built. A post-mortem studies failed or aged cells to find out what went wrong. Many lab steps are the same, but the goal, the samples and the questions in the final report are different.
منتجات وخدمات ذات صلة
استخدم منتجات Canrd وخدمات البحث والتطوير لتحويل معرفة البطاريات إلى تجارب عملية.
علبة coin cell
منتجعلب coin cell للتحقق من المواد والمفاهيم الكهروكيميائية المذكورة في المقالة.
استخدم علب coin cell في اختبارك التالي →إلكتروليت الصوديوم
فئةإلكتروليتات لأبحاث بطاريات الصوديوم-أيون واختبارات التوافق والتحقق من الخلايا.
تصفح إلكتروليت الصوديوم للتحقق →تصنيع الخلايا
خدمةاحصل على دعم لبناء خلايا جافة أو مجمعة أو صيغ مخصصة للتحقق في البحث والتطوير.
اطلب دعم تصنيع الخلايا →مواد تجريبية
فئةتصفح مواد للتجارب اللاحقة والمقارنة وتطوير المنتجات.
تصفح مواد البطاريات التجريبية →