홈/리소스/지식센터/Electrolyte/How to Measure Solid Electrolyte Ionic Conductivity

How to Measure Solid Electrolyte Ionic Conductivity

Canrud November 21, 2026 26

Solid electrolyte ionic conductivity measurement is usually done by pressing the material into a pellet, placing it between two ion-blocking electrodes and running electrochemical impedance spectroscopy (EIS). You read the ionic resistance from the spectrum and convert it to conductivity using the pellet thickness and area.

The formula

σ = L / (R × A)

σ = ionic conductivity (S/cm); L = pellet thickness (cm); R = ionic resistance (Ω); A = electrode contact area (cm²)

 

The method is simple, but small choices change the answer. This guide walks through each step, gives a worked example and lists what to report. If you are still choosing a material, start with our overview of solid electrolyte types for battery research.

What you need before you start

  • A press and die, or a cell that can hold the pellet under a known, controlled pressure.
  • Two ion-blocking electrodes, such as stainless steel or titanium.
  • A potentiostat with impedance capability.
  • A way to control and record temperature.
  • For sulfide electrolytes, an argon glovebox or sealed cell, because they react with moisture.

Sulfides need extra care. Our guide to handling sulfide electrolytes safely covers glovebox limits and hydrogen sulfide risk.

Step 1: Prepare the pellet

Weigh the powder and press it into a dense pellet in a die of known diameter. Measure the final thickness carefully, because thickness appears directly in the formula. Calculate the pellet density from its mass and volume and compare it with the material's theoretical density. A pellet with low density has more pores and gaps between particles, which lowers the measured conductivity.

Step 2: Choose blocking electrodes

Use electrodes that let electrons pass but block lithium ions, such as stainless steel or titanium. Because ions cannot cross into the electrodes, the impedance you measure reflects ion movement through the electrolyte. Good, even contact is essential. Poor contact adds resistance that looks like low conductivity.

Step 3: Set and record stack pressure

Pressure changes the result, often a lot. Higher pressure packs particles more tightly and reduces resistance at grain boundaries. In one published case study, a sulfide electrolyte (LPSC) measured about 0.205 mS/cm at 50 MPa and about 0.819 mS/cm at 350 MPa. A hard oxide (LLZO) changed much less, because oxides deform less than sulfides.

There is no single correct pressure. What matters is to choose one, hold it, and report it with every number.

Step 4: Run the solid electrolyte ionic conductivity measurement (EIS)

Apply a small alternating voltage over a wide frequency range and record the impedance. The case study above used a 10 mV amplitude from 1 MHz down to 0.1 Hz, which is a reasonable starting point. Hold the temperature steady and record it.

To find the activation energy, repeat the measurement at several temperatures and plot the logarithm of conductivity against inverse temperature (an Arrhenius plot). The slope gives the activation energy for ion transport.

Step 5: Read or fit the spectrum

On a Nyquist plot, a pellet between blocking electrodes typically shows one or two arcs followed by a steep line at low frequency. The arcs represent ion movement through the grains (bulk) and across grain boundaries. The steep line comes from the blocking electrodes.

  • Total resistance: read where the arcs end and the steep line begins.
  • Bulk resistance: only possible if the bulk arc is clearly separated, which may need lower temperature or higher frequency.

For complex spectra, fit an equivalent circuit rather than reading points by eye. Our guide to practical EIS data fitting covers the basics.

Step 6: Calculate conductivity (worked example)

Using the published LPSC data point at 50 MPa:

Value

Number

Pellet thickness, L

0.09925 cm

Ionic resistance, R

364.8 Ω

Electrode area, A

1.327 cm² (13 mm diameter)

σ = L / (R × A)

0.09925 / (364.8 × 1.327) = 0.000205 S/cm

Result

about 0.205 mS/cm

 

Keep units consistent: thickness in centimetres and area in square centimetres give S/cm. Multiply by 1,000 for mS/cm.

Common errors that skew results

  • Low pellet density: pores lower conductivity; report density.
  • Poor electrode contact: adds resistance that is not from the electrolyte.
  • Unrecorded pressure: makes the number impossible to compare.
  • Moisture exposure: degrades sulfides before you measure them.
  • Wrong area: use the actual contact area, not the die size, if they differ.
  • Reading the wrong point: confusing bulk, total and electrode features on the plot.

What to report with your number

A conductivity value is only useful with its conditions. Report:

  1. Material, batch and how it was stored.
  2. Pellet mass, thickness, area and relative density.
  3. Stack pressure during measurement.
  4. Temperature.
  5. Electrode material.
  6. Frequency range and amplitude.
  7. Whether the value is bulk or total, and how R was obtained.

Recent work on sulfide electrolytes, such as this 2025 study on robust conductivity determination, shows why these conditions matter when comparing results across labs.

A pellet value is not the same as conductivity inside a working cell, where interfaces and electrode mixtures add resistance. If your result is far from published values for the same material, repeat it with a reference sample before you rely on it.

Pellet, thin film or inside a cell: which measurement do you need?

A pressed pellet is the standard way to compare powders, and it is what this guide covers. Thin films, such as sputtered or cast layers, are measured differently, often with in-plane or interdigitated electrodes. Polymer and composite membranes are usually measured as cut discs between blocking electrodes, without high pressure. Conductivity inside a working cell is different again, because interfaces with electrodes add resistance. Choose the measurement that matches the decision you need to make.

How do you measure activation energy?

Measure conductivity at several temperatures, holding each long enough for the pellet to reach it. Plot the natural logarithm of conductivity (or conductivity multiplied by temperature, depending on the convention you follow) against 1/T in kelvin. The data should fall close to a straight line. The slope equals −Ea/k, where Ea is the activation energy and k is the Boltzmann constant. State which convention you used, because the two give slightly different values.

How do you check that your setup is working?

  • Measure a reference material with a well-established conductivity at the start of a series.
  • Repeat at least one pellet, or remeasure the same pellet after reassembly, to see how much the result varies.
  • Short the cell with blocking electrodes only, to confirm the fixture itself adds little resistance.
  • Check that the pellet thickness after measurement matches the value you used.

These checks take little time and give you confidence that a surprising result comes from the material, not the setup.

Does preparation differ by electrolyte type?

Yes. Sulfide electrolytes are soft and press into dense pellets at room temperature, but must stay in an inert atmosphere. Oxide electrolytes such as garnets are hard, so cold-pressed pellets stay porous; they are usually sintered at high temperature to reach high density before measurement. Polymer electrolytes are measured as films or discs, often at several temperatures. Use the preparation that suits the material, and report it.

Frequently asked questions

Why do labs report different conductivity for the same material?

Because the number depends on how it was measured. Pellet density, stack pressure, temperature, electrode contact and the way resistance is read from the spectrum all change the result. Two careful labs can still disagree if their conditions differ, which is why reporting those conditions matters as much as the value itself.

Should I report bulk or total conductivity?

Report what you measured and say which it is. Total conductivity includes the resistance of grain boundaries between particles and is what a pressed pellet usually gives. Bulk conductivity needs a clearly separated bulk arc in the spectrum, which is often not visible at room temperature for fast conductors.

Can I measure sulfide electrolytes in air?

No. Sulfide electrolytes react with moisture in air, which degrades the material and can release hydrogen sulfide gas. Prepare and measure them in an argon glovebox or a sealed cell that was assembled inside one. Even short exposure can lower the measured conductivity and give a misleading result.

Need an independent conductivity number?

Canrud offers solid electrolyte and separator testing. Tell us the material, its form and the conditions you need, then book a conductivity test. Quoted after a short scope call, all costs listed upfront. More about Canrud R&D.